Measures to Reduce Sticking Phenomenon in 1900 mm Slab Continuous Casting
Author of the article:ZHANG Minghai, ZHAO Jianping, WANG Shuai, TANG Guangpeng, LIU Xin
Author's Workplace:Tangshan Iron and Steel Company, Hebei Iron and Steel Group, Tangshan 063016, China
Key Words:slab caster; sticking; mould protecting slag; sticking times
Abstract:The causes of sticking phenomenon in 1 900 mm slab continuous casting were analyzed. The results show that
the main reason of sticking is that the protective slag between the green shell and the copper plate can not play a good
lubrication and heat transfer function. Slag by optimizing performance, change the mold copper plate coating material,
waterproofing crystallizer, choosing the right at the bottom of the nozzle immersion depth and nozzle angle, choosing
appropriate three-way argon flow, standardization of pouring molten steel superheat control, constant speed, standardize the
worker operation measures, such as 1 900 mm slab continuous caster sticking number by 20 times down to 4 times a month.